All products
Flagship platforms
Full range
Explore
Get in touch

Light soaking, metastability and preconditioning of PV modules

Light soaking exposes a module to controlled light under load until its power stops changing, so that a rating describes a defined state; IEC 61215 sets the criterion per technology (for crystalline silicon at least 10 kWh/m² in two intervals and a 1 % criterion [1]), thin-film and perovskite devices need more care because their state also depends on temperature, bias and dark time [2], and current injection is acceptable only once validated against light.

The measurement problem

A module measured straight out of storage may be in a state it never has in the field. For thin film, preconditioning is the dominant cause of disagreement between reference laboratories [3]; for TOPCon after UV exposure, dark-storage metastability can be read as degradation [4].

The physics behind it

  • Crystalline silicon: boron-oxygen light-induced degradation and LeTID [5]; stabilisation research for IEC 61215 [6].
  • Amorphous silicon: Staebler-Wronski degradation, partly reversible by annealing [7].
  • CdTe and CIGS: reversible changes with light, bias and temperature, relaxation in the dark [8]; the light-stabilised state depends on exposure temperature [2].
  • TOPCon after UV: a metastable dark loss recovering within minutes under light [9].
  • Perovskite: ion migration over seconds to minutes and fatigue over light-dark cycles [10].

What the measurement must achieve

  • Use the stabilisation of the technology-specific part of IEC 61215 or a validated alternative, and report it.
  • Control the module temperature during exposure and record it.
  • Fix the delay between the end of exposure and the flash.
  • Validate any bias-based method against light stabilisation for each product [11].
  • Monitor irradiance stability during the soak: IEC 60904-9 defines long-term instability for irradiation exposure from at least 100 readings [12].

Applicable standards

Applicable standards
StandardWhat it governs here
IEC 61215-2:2021Terrestrial PV modules, design qualification and type approval: test proceduresMQT 19 stabilisation: light-induced and other procedures, initial and final stabilisation, BO-LID.
IEC 61215-1-1:2021Special requirements for crystalline silicon modulesc-Si criterion x = 0.01, initial stabilisation at least 10 kWh/m² in two intervals of at least 5 kWh/m².
IEC 61215-1-2:2021Special requirements for thin-film cadmium telluride (CdTe) modulesCdTe stabilisation.
IEC 61215-1-3:2021Special requirements for thin-film amorphous silicon modulesAmorphous silicon stabilisation.
IEC 61215-1-4:2021Special requirements for thin-film Cu(In,Ga)(S,Se)2 (CIGS) modulesCIGS stabilisation and dark-soak rules.
IEC 60904-9:2020 (edition 3)Classification of solar simulator characteristicsLong-term instability for irradiation exposure.
ISOS protocols (Khenkin et al., 2020)Consensus statement for stability assessment and reporting of perovskite photovoltaic devicesLight-soaking protocols (ISOS-L) for perovskite stability.

Measurement technologies: advantages and limitations

Steady-state light sources (LED or lamps) perform the soak; LED offers closed-loop irradiance and a stable spectrum, lamps a broadband spectrum including UV, which matters where recovery is wavelength dependent [13]. Current injection in the dark is fast and weather independent: it held CIGS modules within 1 % [14], while one bias-only method failed validation on CdTe [11]. The I-V measurement after the soak can be pulsed or steady state.

Where Pasan equipment fits

  • LED Light SoakerContinuous, closed-loop regulated LED light on full-size modules, MPP, short-circuit or open-circuit bias, 1 Hz log of current, voltage and irradiance, programmable soak steps.
  • HighLIGHT 100ms LabOptional current-injection preconditioning with the flash a fraction of a second after the injection (CdTe).

Technical questions

What does MQT 19 require for crystalline silicon?
At least 10 kWh/m² of light exposure, in two intervals of at least 5 kWh/m², until the power changes by less than 1 % (criterion x = 0.01) [1].
Is current injection an alternative to light soaking?
Only once validated against light stabilisation for that product. It worked for CIGS [14]; one method failed for CdTe [11].
Does the temperature during soaking matter?
Yes, for thin film the stabilised state can differ by 5.8 % for 20 °C [2].

References

  1. IEC, “IEC 61215-1:2021, IEC 61215-1-1:2021 and IEC 61215-2:2021, Terrestrial photovoltaic modules: design qualification and type approval”, International Electrotechnical Commission, 2021. Source
  2. M. G. Deceglie, T. J. Silverman, B. Marion, S. R. Kurtz, “Temperature-dependent light-stabilized states in thin-film PV modules”, 42nd IEEE Photovoltaic Specialists Conference, 2015. doi:10.1109/PVSC.2015.7355854
  3. E. Salis, D. Pavanello, M. Field et al., “Improvements in world-wide intercomparison of PV module calibration”, Solar Energy 155, 1451-1461, 2017. doi:10.1016/j.solener.2017.07.081
  4. P. Gebhardt et al., “UV-induced degradation: comparative analysis of PV module testing and stabilization procedures against outdoor behavior”, EPJ Photovoltaics 17, 15, 2026. doi:10.1051/epjpv/2026007
  5. D. Chen et al., “Progress in the understanding of light- and elevated temperature-induced degradation in silicon solar cells: a review”, Progress in Photovoltaics 29, 1180-1201, 2021. doi:10.1002/pip.3362
  6. I. L. Repins et al., “Stabilization of light-induced effects in Si modules for IEC 61215 design qualification”, Solar Energy 208, 894-904, 2020. doi:10.1016/j.solener.2020.08.025
  7. D. L. Staebler, C. R. Wronski, “Reversible conductivity changes in discharge-produced amorphous Si”, Applied Physics Letters 31, 292-294, 1977. doi:10.1063/1.89674
  8. C. Deline, J. del Cueto, D. S. Albin, S. Rummel, “Metastable electrical characteristics of polycrystalline thin-film photovoltaic modules upon exposure and stabilization”, Journal of Photonics for Energy 2, 022001, 2012. doi:10.1117/1.JPE.2.022001
  9. D. B. Kern et al., “UV-induced degradation and associated metastability in TOPCon photovoltaic modules: understanding kinetics and cell variance”, Progress in Photovoltaics 34, 589-599, 2026. doi:10.1002/pip.70067
  10. M. V. Khenkin et al., “Consensus statement for stability assessment and reporting for perovskite photovoltaics based on ISOS procedures”, Nature Energy 5, 35-49, 2020. doi:10.1038/s41560-019-0529-5
  11. M. G. Deceglie, T. J. Silverman, B. Marion, S. R. Kurtz, “Robust measurement of thin-film photovoltaic modules exhibiting light-induced transients”, Proc. SPIE 9561, 956108, 2015. doi:10.1117/12.2188827
  12. IEC, “IEC 60904-9:2020, Photovoltaic devices, Part 9: Classification of solar simulator characteristics (edition 3.0)”, International Electrotechnical Commission, 2020. Source
  13. D. Zubieta Sempertegui et al., “Metastable dark degradation and light recovery in UV exposed commercial TOPCon”, Solar Energy Materials and Solar Cells 307, 114627, 2026. doi:10.1016/j.solmat.2026.114627
  14. C. Deline et al., “Electrical bias as an alternate method for reproducible measurement of CIGS photovoltaic modules”, Proc. SPIE 8472, 84720G, 2012. doi:10.1117/12.929899
Related pages
Guide: light soaking PV modulesFirst Solar CdTeDegradation and reliability

How this page is written: claims about physics and standards cite published sources, claims about Pasan equipment repeat only what the product pages state, and no other manufacturer is named. Editorial method