Measuring First Solar CdTe modules (Series 4, 6 and 7): what the evidence says

Measuring a First Solar CdTe module accurately is mainly a preconditioning problem, not a light-source problem: the module's power depends on its recent light, bias and temperature history by several percent [1][2], so it must be stabilised under controlled conditions (IEC 61215-1-2, or a current-injection procedure validated against light) and measured at a fixed delay, against a CdTe reference or with a full IEC 60904-7 spectral mismatch correction; once the module is in a defined state, the published evidence shows no accuracy advantage of steady-state light or long pulses for the I-V itself [3].

The measurement problem

First Solar is by far the largest maker of cadmium telluride (CdTe) modules, and its Series 6 and Series 7 modules reach test laboratories from factories, power plants, banks' technical advisers and round robins. They are measured on the same flashers as crystalline silicon, but they behave differently. Reference laboratories agree that the dominant source of disagreement between them is not the simulator but how the module was treated before the flash: in a four-laboratory worldwide intercomparison, the authors named preconditioning "the most critical factor for obtaining consistent results" [4].

First Solar's public documents rate modules at STC with a 0/+5 % power tolerance and describe the ratings as "as received and stabilized" [5], but give no flash-test or preconditioning procedure. This page summarises what independent research says, so that a laboratory can build a procedure it can defend.

The physics behind it

Metastability

CdTe devices are metastable: their open-circuit voltage and fill factor change with light exposure, electrical bias and temperature, and relax back in the dark. In NREL measurements, light exposure moved the maximum power of CdTe modules in both directions and by up to 16 %, driven by Voc and fill factor [1]. Light-induced Voc transients with a time constant of about 1.1 h were observed on commercial modules [6], and relaxation after stabilisation can take weeks [2]. Copper at the back contact is widely understood to drive much of this behaviour [1].

The stabilised state itself depends on temperature during exposure: one CdTe product varied by 5.8 % for a 20 °C change in exposure temperature, and the authors concluded that a unique light-soaked state is poorly defined for CdTe and CIGS [7].

CdSeTe absorbers and arsenic doping (CuRe)

Selenium alloying (CdSeTe) lowers the front band gap from about 1.5 eV to about 1.4 eV and extends collection into the red [8]. A review co-authored by First Solar staff states that arsenic-doped CdSeTe modules (Series 6 CuRe) are in production, and that group-V doped modules "have simply not been studied long enough" for a large body of stability literature [9]. Almost all published module metastability data concern earlier copper-doped products, so behaviour of current Series 6 CuRe and Series 7 modules must be verified, not assumed.

Spectral response

CdTe responds over roughly 300 to 900 nm [2], while a crystalline silicon reference cell responds up to about 1200 nm. Simulator light between 900 and 1200 nm is therefore seen by a silicon reference but not by the module. No public module-level quantum efficiency of Series 6 or 7 was found; a 2026 Sandia study had to use a Series 4 curve because a Series 6 one was not available [10].

Capacitance and sweep time

Monolithic series connection keeps the module capacitance small, equivalent to that of a cell of about 0.5 to 2 cm² [11]. Sweep times longer than about 1 ms did not change the measured power of CdTe and CIGS modules in a systematic study [3], and the JRC found no sweep-time effect for CdTe [12]. Cell-level hysteresis exists in copper-doped devices, but its effect on maximum power was small [13]. No public sweep-time study on Series 6 CuRe or Series 7 was found.

What the measurement must achieve

  • Store modules in the dark at or below 25 °C and record the storage time: IEC 61215-1-2 requires it, because dark storage changes the power [2].
  • Bring the module to a defined state: light stabilisation in at least two intervals of 20 kWh/m² each until the power changes by less than 2 % (IEC 61215-1-2:2016), or a current-injection procedure validated against light stabilisation for that product [14].
  • Control and report the temperature during exposure, since the stabilised state depends on it [7].
  • Measure at a fixed, documented delay after exposure: NREL's protocol cools to 25 °C and completes the I-V within 0.5 to 1 h [14]; for in-line current injection, keep the delay between the end of injection and the flash identical for every module.
  • Use a CdTe reference module of the same product calibrated by an accredited laboratory, or a silicon reference with a full IEC 60904-7 correction using the module's measured spectral responsivity and the simulator spectrum [15].
  • Control the module temperature to 25 ± 1 °C or correct with the product's coefficients (about -0.3 %/°C for Pmax on Series 6 and 7 datasheets [16]).
  • Check each new product at two sweep durations and in both sweep directions; differences should stay within the system's repeatability.

Applicable standards

Applicable standards
StandardWhat it governs here
IEC 61215-1-2:2021Special requirements for thin-film cadmium telluride (CdTe) modulesCdTe-specific stabilisation: dark storage below 25 °C, light exposure in intervals of at least 20 kWh/m² to a 2 % criterion, power measurement 30 to 60 min after exposure in the 2016 edition, validated alternative procedures allowed.
IEC 61215-2:2021Terrestrial PV modules, design qualification and type approval: test proceduresMQT 19 stabilisation and MQT 06 performance at STC; bias-based stabilisation only after validation.
IEC 60904-7:2019Computation of the spectral mismatch correctionSpectral mismatch correction between the CdTe module and a reference device with different spectral responsivity.
IEC 60904-8:2014Measurement of spectral responsivity of a PV deviceMeasurement of the module's spectral responsivity, needed for the mismatch correction.
IEC 60904-1:2020Measurement of photovoltaic current-voltage characteristicsI-V measurement under simulated sunlight, including the sweep.
IEC 60904-2:2023Requirements for photovoltaic reference devicesRequirements for the reference device, including a matched CdTe reference module.
IEC 60891:2021Procedures for temperature and irradiance corrections to measured I-V characteristicsTemperature and irradiance corrections when the module is not at exactly 25 °C and 1000 W/m².
IEC 60904-9:2020 (edition 3)Classification of solar simulator characteristicsClassification of the simulator; spectral match over 300 to 1200 nm matters less than mismatch correction for CdTe.

Measurement technologies: advantages and limitations

Two requirements are often confused. Preconditioning needs a sustained dose of light or a validated bias, applied before the measurement. The I-V measurement needs a stable, well-characterised light for long enough to sweep a low-capacitance device. A light source can be good at one and irrelevant to the other.

Light sources for CdTe module measurement
TechnologyFor preconditioningFor the I-V measurementLimitations
Short-pulse xenon (a few ms)Not suitableUsed by reference laboratories on stabilised CdTe [17]; no sweep-time effect above about 1 ms [3]Spectral mismatch must be corrected; flash-to-flash stability must be monitored
Long-pulse xenon (tens of ms)Not suitableAdequate for CdTe; the longer plateau is needed for capacitive silicon, not for CdTeSame spectral correction as any xenon source
Steady-state xenon or LEDSuitable when temperature is controlledSuitable, but heats the module and can keep changing its state while it is measuredNo published evidence of better CdTe I-V accuracy [3]
LED (pulsed or steady)Steady LED suitableSpectrum can be tuned to reduce mismatch: so far shown by modelling [18]No measured module-level CdTe comparison with xenon found
Current injection in the darkFast and weather-independent once validated per product [14]Not a light sourceBias-only methods can differ from light stabilisation by several percent [1]
Mismatch magnitudes are properties of a specific simulator spectrum and reference device, not of xenon or LED in general: a NIST example gave a mismatch factor of 1.034 under one xenon flash and 1.103 under one steady-state xenon simulator, the difference being due to filtering [19].

Where Pasan equipment fits

  • HighLIGHT 100ms LabLong-pulse xenon module simulator, A+A+A+ to IEC 60904-9. CdTe modules, First Solar's included, are measured after current-injection preconditioning, the flash following the injection by a fraction of a second; the integrated filter set gives module-level spectral response for the mismatch correction.
  • HighLIGHT 100ms ProdThe same measurement core on the production line, at about 15 s per module.
  • LED Light SoakerContinuous, closed-loop regulated LED light with MPP, short-circuit or open-circuit load bias for IEC 61215 MQT 19 stabilisation, and a full exposure log per module.
  • Nexun LED simulators (Avalon ST)Full-LED simulators of Pasan's sister company, which also measure CdTe modules.

Current injection: fast, but validate it

Driving the module with a forward current in the dark reaches a repeatable state in minutes and fits on the flasher. It is not automatically equivalent to light soaking. NREL tested a draft method (forward bias at 85 °C) on four CdTe modules: on its own it differed from a subsequent light stabilisation by 2.2 to 3.8 % and was rejected, while bias followed by light agreed within 0.1 to 1.0 % [14]. Modules that moved in opposite directions under light moved the same way under that bias method [1]. Earlier NREL work at 65 °C found that light or dark bias could both stabilise the products tested, to varying degrees [11], and PTB has proposed the dark I-V curve as a fingerprint of the module's state [20].

  1. Light-stabilise three modules of the product and measure them (the reference state).
  2. Let them relax in the dark, then apply the current-injection recipe and measure with the production timing.
  3. Accept the recipe if the two results agree within the criterion you will report (2 % in the IEC 61215 validation logic [14]), and repeat when the product changes.

Realistic uncertainty

Fraunhofer ISE's CalLab reported an expanded uncertainty of 2.9 % (k = 2) for CdTe module power, against 1.6 % for its best crystalline silicon case, naming spectral mismatch and short-term stability as the differences [21]. The choice between a filtered and an unfiltered silicon reference moved CdTe Isc by 1.1 % on average, while CdTe reference modules agreed within 0.5 % [15]. Agreement between reference laboratories on thin film improved from 3 to 6 % around 2010 [2] to about ±1 to 2 % in 2017 [4]; a 2015 European intercomparison saw -7.9 % to +11.9 % for preconditioned CdTe [22].

Independent evidence

  • Preconditioning is the main cause of disagreement between reference laboratories on thin-film modules [4][22].
  • No sweep-time effect on CdTe modules above about 1 ms [3][12].
  • Bias-only stabilisation can differ from light stabilisation by 2.2 to 3.8 %; bias plus light agreed within 1 % [14].
  • Temperature coefficients measured during warm-up under continuous light are contaminated by light-induced transients; indoor flash measurements during cool-down avoided this [6].
  • PI Berlin described measuring thin-film modules, CdTe among them, on a Pasan SunSim IIIb with partial traces inside its 8 ms sweep [23].

Technical questions

What is the best solar simulator for First Solar modules?
Any IEC 60904-9 class A or A+ simulator that can measure a large high-voltage module can rate a First Solar module correctly, provided the module is stabilised under controlled conditions and the spectral mismatch is corrected. The procedure matters more than the lamp: preconditioning is the main cause of disagreement between laboratories [4].
Do CdTe modules need a long pulse or steady-state light for the I-V curve?
No published evidence says so. Sweeps longer than about 1 ms did not change the measured power of CdTe modules [3], and reference laboratories have measured stabilised CdTe with pulses of a few milliseconds. Sustained light is needed for preconditioning, which is a separate step.
Is current injection equivalent to light soaking for CdTe?
Not automatically. It can reach a repeatable state in minutes, but one bias-only method differed from light stabilisation by 2.2 to 3.8 % on four CdTe modules [14]. Validate the recipe per product against light stabilisation.
How long after preconditioning should a CdTe module be measured?
At a short, fixed delay. NREL's protocol completes the I-V within 0.5 to 1 h after light exposure, after cooling to 25 °C [14]; IEC 61215-1-2:2016 measures 30 to 60 min after exposure. With in-line current injection, flash at the same delay for every module.
Can a silicon reference cell be used for CdTe?
Yes, with a full IEC 60904-7 spectral mismatch correction based on the module's measured spectral responsivity and the simulator spectrum. A CdTe reference module of the same product gave the most consistent results in a published comparison [15].
What uncertainty can a laboratory achieve on CdTe module power?
Fraunhofer ISE CalLab reported 2.9 % (k = 2) for CdTe [21]; IEC 61215-1-2:2021 accepts up to 4.0 % for single-junction CdTe. Uncontrolled preconditioning can add several percent on its own.

References

  1. T. J. Silverman, M. G. Deceglie, B. Marion, S. R. Kurtz, “Performance stabilization of CdTe PV modules using bias and light”, IEEE Journal of Photovoltaics 5(1), 344-349, 2015. doi:10.1109/JPHOTOV.2014.2370252
  2. T. J. Silverman, U. Jahn, G. Friesen et al., “Characterisation of performance of thin-film photovoltaic technologies”, IEA PVPS Task 13, Report IEA-PVPS T13-02:2014, 2014. Source
  3. J. Kuurne, A. Tolvanen, J. Hyvärinen, “Sweep time, spectral mismatch and light soaking in thin film module measurement”, 33rd IEEE Photovoltaic Specialists Conference, 2008. doi:10.1109/PVSC.2008.4922583
  4. E. Salis, D. Pavanello, M. Field et al., “Improvements in world-wide intercomparison of PV module calibration”, Solar Energy 155, 1451-1461, 2017. doi:10.1016/j.solener.2017.07.081
  5. First Solar, “Series 6 modules user guide, PD-5-200-06 Rev 7.0 (retrieved November 2026)”, First Solar technical documents, 2026. Source
  6. C. Deline, J. del Cueto, D. S. Albin et al., “Transient response of cadmium telluride modules to light exposure”, 37th IEEE Photovoltaic Specialists Conference, 2011. doi:10.1109/PVSC.2011.6186602
  7. M. G. Deceglie, T. J. Silverman, B. Marion, S. R. Kurtz, “Temperature-dependent light-stabilized states in thin-film PV modules”, 42nd IEEE Photovoltaic Specialists Conference, 2015. doi:10.1109/PVSC.2015.7355854
  8. X. Zheng, D. Kuciauskas, J. Moseley et al., “Recombination and bandgap engineering in CdSeTe/CdTe solar cells”, APL Materials 7, 071112, 2019. doi:10.1063/1.5098459
  9. M. A. Scarpulla, B. McCandless, A. B. Phillips et al., “CdTe-based thin film photovoltaics: recent advances, current challenges and future prospects”, Solar Energy Materials and Solar Cells 255, 112289, 2023. doi:10.1016/j.solmat.2023.112289
  10. A. R. Jensen, K. S. Anderson, B. H. King, “Shading effects of thin-film photovoltaic modules”, IEEE Journal of Photovoltaics 16(5), 2026. doi:10.1109/JPHOTOV.2026.3702674
  11. J. A. del Cueto, C. A. Deline, S. R. Rummel, A. Anderberg, “Progress toward a stabilization and preconditioning protocol for polycrystalline thin-film photovoltaic modules”, 35th IEEE Photovoltaic Specialists Conference, 2010. doi:10.1109/PVSC.2010.5614223
  12. A. Virtuani, H. Müllejans, E. D. Dunlop, “Comparison of indoor and outdoor performance measurements of recent commercially available solar modules”, Progress in Photovoltaics 19(1), 11-20, 2011. doi:10.1002/pip.977
  13. D. S. Albin, J. A. del Cueto, “Effect of hysteresis on measurements of thin-film cell performance”, Proc. SPIE 7773, 77730N, 2010. doi:10.1117/12.861175
  14. M. G. Deceglie, T. J. Silverman, B. Marion, S. R. Kurtz, “Robust measurement of thin-film photovoltaic modules exhibiting light-induced transients”, Proc. SPIE 9561, 956108, 2015. doi:10.1117/12.2188827
  15. L. Pratt, N. Riedel, M. Yamasaki, M. F. Plass, “The components of variance for calibration methods of thin film CdTe photovoltaic modules”, 39th IEEE Photovoltaic Specialists Conference, 2013. doi:10.1109/PVSC.2013.6744232
  16. First Solar, “Series 7 TR1 datasheet, MPD-00640-07-US”, First Solar technical documents, 2026. Source
  17. T. Sample (JRC ESTI), “Preconditioning of thin-film PV modules through controlled light-soaking”, NREL PV Module Reliability Workshop, 2012. Source
  18. Ž. Vosylius, A. Novičkovas, V. Tamošiūnas, “Optimization of LED-based solar simulators for cadmium telluride and microcrystalline silicon solar cells”, Energies 16, 5741, 2023. doi:10.3390/en16155741
  19. B. H. Hamadani, B. Dougherty, “Solar cell characterization”, Semiconductor Materials for Solar Photovoltaic Cells, Springer Series in Materials Science, 2016. doi:10.1007/978-3-319-20331-7_8
  20. B. Friedel, S. Winter, “Alternative preconditioning by utilization of a thin film module's dark diode fingerprint”, EPJ Photovoltaics 15, 3, 2024. doi:10.1051/epjpv/2023033
  21. D. Dirnberger, U. Kräling, “Uncertainty in PV module measurement, part I: calibration of crystalline and thin-film modules”, IEEE Journal of Photovoltaics 3(3), 1016-1026, 2013. doi:10.1109/JPHOTOV.2013.2260595
  22. B. Mihaylov, J. W. Bowers, T. R. Betts et al., “Results of the SOPHIA module intercomparison part 2: STC, low irradiance conditions and temperature coefficients measurements of thin film technologies”, 31st European PV Solar Energy Conference, 2015. doi:10.4229/EUPVSEC20152015-5DO.11.2
  23. P. Grunow, A. Preiss, M. Schoppa, S. Krauter, “Actual issues on power measurement of photovoltaic modules”, Photovoltaics International, 8th edition, 2010. Source
Related pages
CdTe solar simulatorsLight soaking and metastabilitySpectral mismatch correctionGuide: current-injection preconditioningThin-film module measurement

How this page is written: claims about physics and standards cite published sources, claims about Pasan equipment repeat only what the product pages state, and no other manufacturer is named. Editorial method

Rather we contact you?

Leave your email and we will get back to you. No form to fill in.

We only use your address to answer you. Privacy policy