Thin-film PV module measurement: CdTe, CIGS and amorphous silicon

Thin-film modules differ from crystalline silicon in three ways that decide a measurement: each technology has its own stabilisation (light-induced degradation for amorphous silicon, reversible metastability for CdTe and CIGS), their spectral responses differ strongly from a silicon reference so mismatch must be corrected, and amorphous silicon, unlike CdTe and CIGS, shows sweep-time effects [1][2].

The measurement problem

Thin-film round robins have historically agreed less well than crystalline silicon ones: within 3 to 6 % among European laboratories around 2010, depending on technology [1], against about ±1.3 % for crystalline silicon among four reference laboratories [3]. The causes are known and controllable.

The physics behind it

  • Amorphous and microcrystalline silicon lose efficiency under light (Staebler-Wronski effect) until they reach a stabilised level; annealing at temperature partly reverses it [1].
  • CdTe and CIGS are metastable in both directions: light, bias and heat move their power up or down, and dark storage moves it back [4][5].
  • Spectral response bands differ from silicon (about 300 to 900 nm for CdTe [1]), so a silicon reference needs a mismatch correction.
  • Amorphous silicon shows appreciable sweep-time effects; CdTe and CIGS did not in JRC tests [2], nor above about 1 ms in a manufacturer study [6].

What the measurement must achieve

  • Apply the stabilisation of the technology-specific part of IEC 61215 (or a validated alternative) and report it.
  • Control storage, transport and the delay between stabilisation and measurement [7].
  • Correct spectral mismatch with measured spectral responsivity, or use a matched reference module.
  • For amorphous silicon, verify that the sweep is slow enough (or use a multi-segment method).
  • Record temperature during stabilisation as well as during measurement [5].

Applicable standards

Applicable standards
StandardWhat it governs here
IEC 61215-1-2:2021Special requirements for thin-film cadmium telluride (CdTe) modulesCdTe-specific requirements and stabilisation.
IEC 61215-1-3:2021Special requirements for thin-film amorphous silicon modulesAmorphous silicon specific requirements and stabilisation.
IEC 61215-1-4:2021Special requirements for thin-film Cu(In,Ga)(S,Se)2 (CIGS) modulesCIGS specific requirements and stabilisation.
IEC 61215-2:2021Terrestrial PV modules, design qualification and type approval: test proceduresMQT 19 stabilisation procedure.
IEC 60904-7:2019Computation of the spectral mismatch correctionSpectral mismatch correction.
IEC 60904-1:2020Measurement of photovoltaic current-voltage characteristicsI-V measurement, including sweep requirements.

Measurement technologies: advantages and limitations

Pulsed simulators measure stabilised thin-film modules well when the sweep is long enough for the technology (amorphous silicon is the demanding case). Steady-state sources combine stabilisation and measurement but heat the module and may change its state during the sweep. The stabilisation itself is a dose of light or a validated bias, best done in a regulated light soaker or under a documented outdoor procedure.

Where Pasan equipment fits

Technical questions

Why do thin-film modules need stabilisation?
Because their power changes with exposure: amorphous silicon degrades under light until it stabilises, and CdTe and CIGS move up or down with light, bias and heat. Without stabilisation the rating describes a temporary state [1].
Which thin-film technology is sensitive to sweep time?
Amorphous silicon. JRC found no sweep-time effect for CdTe and CIS modules [2].
How well do laboratories agree on thin-film modules?
Among reference laboratories, about ±1 to 2 % in 2017, with most inconsistencies traced to preconditioning [8].

References

  1. T. J. Silverman, U. Jahn, G. Friesen et al., “Characterisation of performance of thin-film photovoltaic technologies”, IEA PVPS Task 13, Report IEA-PVPS T13-02:2014, 2014. Source
  2. A. Virtuani, H. Müllejans, E. D. Dunlop, “Comparison of indoor and outdoor performance measurements of recent commercially available solar modules”, Progress in Photovoltaics 19(1), 11-20, 2011. doi:10.1002/pip.977
  3. D. Dirnberger, U. Kräling, H. Müllejans et al., “Progress in photovoltaic module calibration: results of a worldwide intercomparison between four reference laboratories”, Measurement Science and Technology 25, 105005, 2014. doi:10.1088/0957-0233/25/10/105005
  4. T. J. Silverman, M. G. Deceglie, B. Marion, S. R. Kurtz, “Performance stabilization of CdTe PV modules using bias and light”, IEEE Journal of Photovoltaics 5(1), 344-349, 2015. doi:10.1109/JPHOTOV.2014.2370252
  5. M. G. Deceglie, T. J. Silverman, B. Marion, S. R. Kurtz, “Temperature-dependent light-stabilized states in thin-film PV modules”, 42nd IEEE Photovoltaic Specialists Conference, 2015. doi:10.1109/PVSC.2015.7355854
  6. J. Kuurne, A. Tolvanen, J. Hyvärinen, “Sweep time, spectral mismatch and light soaking in thin film module measurement”, 33rd IEEE Photovoltaic Specialists Conference, 2008. doi:10.1109/PVSC.2008.4922583
  7. M. G. Deceglie, T. J. Silverman, B. Marion, S. R. Kurtz, “Robust measurement of thin-film photovoltaic modules exhibiting light-induced transients”, Proc. SPIE 9561, 956108, 2015. doi:10.1117/12.2188827
  8. E. Salis, D. Pavanello, M. Field et al., “Improvements in world-wide intercomparison of PV module calibration”, Solar Energy 155, 1451-1461, 2017. doi:10.1016/j.solener.2017.07.081
Related pages
First Solar CdTe modulesCIGS modulesLight soaking and metastability

How this page is written: claims about physics and standards cite published sources, claims about Pasan equipment repeat only what the product pages state, and no other manufacturer is named. Editorial method